Home / Application Guide / Quality & Defects

Conformal Coating Application Guide

Characteristics of each dispensing valve, a comparison of six resin chemistries, and quality checks and defect prevention on the shop floor.For product-specific conditions, follow the relevant TDS.

Shop-floor quality checks and common defect fixes

The keys are letting the coating reach room temperature after delivery, allowing flash-off before curing, and keeping the board surface clean and dry.

Defect example photo

Cobwebbing

Main causes

When a solvent-based coating is sprayed with air, the solvent flashes off rapidly at the nozzle tip and droplets tangle into threads.

Prevention

Lower the atomizing air pressure and the nozzle-to-board distance. Use a viscosity setting matched to your spray valve.

Defect example photo

Orange Peel

Main causes

The surface turns bumpy like orange skin when the film is too thick, the board is warmer than the coating, or the spray pressure is low with the nozzle at an angle.

Prevention

Keep to the recommended thickness and match the board and coating temperatures. Set the spray pressure correctly and keep the nozzle perpendicular to the board.

Defect example photo

Bubbles & Pinholes

Main causes

If the board goes into a hot curing oven without enough flash-off right after coating, the surface skins over first and traps gas inside.

Prevention

Let the container reach the room temperature of your workshop before use. Allow enough room-temperature flash-off time before hot-air curing.

Defect example photo

Keep-out Violation / Wicking

Main causes

Masking is missed on areas that must stay uncoated, such as connector pins and test points, or the coating wicks under components and into connectors by capillary action.

Prevention

Block keep-out areas on the drawing with masking or boots. Control boundaries with a needle or jetting valve dam and a matched viscosity.

Defect example photo

De-wetting

Main causes

Flux, release agents, oil or fingerprints left on the board surface make the coating pull away.

Prevention

Check board cleaning and drying before coating. Test no-clean fluxes for compatibility with the coating first.

Defect example photo

Fish-eyes

Main causes

Spot contamination such as silicone, wax, rework residue or dust pushes the coating away in a circle, leaving a hole.

Prevention

Clean boards before coating and remove residue from temporary masking. Control silicone release agents and lubricants around the coating area.

Defect example photo

Blushing

Main causes

In hot, humid conditions, evaporating solvent cools the surface and moisture from the air condenses on it, turning it cloudy.

Prevention

Control the relative humidity of the coating booth and curing area. Remove moisture absorbed by the board by pre-baking.

Defect example photo

Incomplete Cure

Main causes

The film stays tacky when cure temperature or time is too short, a moisture-cure product is cured in low humidity, or shadow areas the UV cannot reach remain.

Prevention

Follow the cure conditions (temperature, time, humidity) in the TDS. For UV-cure products, check the UV dose and the cure of shadow areas.

Defect example photo

Cracking

Main causes

Applying too thick a film at once or drying it quickly at high temperature cures it unevenly, so it cracks. Severe thermal shock can also cause it.

Prevention

Apply within the recommended thickness and follow the cure temperature in the TDS. Consider a more flexible coating for environments with severe thermal shock.

Defect example photo

Delamination

Main causes

Surface contamination such as silicone or flux residue, poor adhesion to the solder resist, or excessive thickness makes the film lift off the board.

Prevention

Remove surface contamination by cleaning and apply several thin coats. Apply the next coat only after the previous one is dry to the touch.

Defect names and items are based on the coating-related content of IPC-A-610 (Acceptability of Electronic Assemblies) and IPC J-STD-001. Actual acceptance criteria follow your drawings and specifications.

Wondering which resin and viscosity suit your current equipment?

Tell us the valves you use and your curing conditions, and we'll recommend suitable products and send the TDS.

Request a process consultation
Product photo coming soon

Viscosity is for the product as supplied (standard specification). Conformal coatings can also be shipped pre-set to the viscosity (cP) your equipment needs.